    The company produces and sells "Yuanzheng" brand matting powder (MATTING AGENT)
    News
    Home > News
    Research on cryogenic treatment process of powder metallurgy parts shaping mold
    Time:2022-03-20

    Research on cryogenic treatment technology of powder metallurgy parts shaping die

            Powder metallurgy parts are more and more widely used in machinery and other industries due to their inherent advantages. The production process of powder metallurgy parts is generally as follows: powder compaction - high temperature pouring - shaping. The reshaped powder metallurgy parts can be directly equipped with a little machining. Therefore, there are strict requirements on the dimensional tolerances of the reshaped parts. In order to ensure the dimensional requirements of the powder metallurgy parts, the dimensional tolerances of the female mold and the mandrel of the shaping die are required. The requirements are more stringent, such as the size of the shaping mandrel for a certain bushing is Ф20+0.025. The female die and the mandrel are subjected to a large extrusion force during the shaping process, and the working conditions are very bad, and it is easy to be scrapped due to the excessive size caused by severe wear. Therefore, improving the wear resistance of powder metallurgy parts shaping molds, thereby improving the life of shaping molds, is of great significance to the quality of powder metallurgy parts and reducing the production cost of powder metallurgy parts. This paper intends to discuss the cryogenic treatment process to improve the life of powder metallurgy parts shaping die through the cryogenic treatment of powder metallurgy parts shaping mandrel.


    1 Test method
    Take a batch of machined 132 bushing shaping mandrels from a powder metallurgy factory, and the mandrel material is GCr15. After normal quenching and low temperature tempering at 150℃, the mandrel rod should be cryogenically treated as soon as possible. 1h, 2h, 4h, and 8h 4 times. The molds after cryogenic treatment were all tempered at a temperature lower than 150 °C, and the holding time was 1 h, and their hardness was measured respectively. The cryogenically treated mandrel and the same batch of heat-treated mandrels without cryogenic treatment were installed on the machine to measure their life, and the wear patterns of the molds with different treatment processes were observed with a low magnification magnifying glass.


    2 Test results and analysis


    2.1 Test results


    Table 1 Life and hardness of mandrel after different treatments

    Cryogenic treatment temperature (℃)

    Cryogenic treatment holding time (h)

    Average service life
    (Number of plastic parts)

    average hardness(HPC)

    -100

    1

    3800

    60.5

    2

    4100

    60.6

    4

    4300

    61

    8

    4500

    61.5

    -120

    1

    4400

    60.5

    2

    4800

    61

     

    5100

    61

     

    5300

    61.5

    -140

    1

    5200

    61

    2

    5500

    61.5

    4

    5800

    61.5

    8

    6100

    62

    -160

    1

    5900

    62

    2

    6600

    62

    4

    6900

    62

    8

    7100

    62

    -196

    1

    6300

    62

    2

    6800

    62

    4

    7100

    62

    8

    7200

    62

    Not cryogenically treated

     

    3000

    60.5

    It can be seen from Table 1 that the service life of the powder metallurgy parts shaping mandrel is significantly improved after cryogenic treatment. The lower the cryogenic temperature and the longer the holding time, the more parts are reshaped before the mold fails, that is, the longer the service life of the mold. However, when the holding time is the same, the lifespan of the shaping mandrel at -160℃ and -196℃ is not much different. At the same processing temperature, when the holding time exceeds two hours, the mold life jumps up, and then increases smoothly with the extension of the holding time.

    2.2 Analysis of test results

    Observing the surface of the failed shaping mold, it was found that the surface of the mold was covered with spalling pits and many small furrows. This is due to the fact that during the shaping process of the mold, the powder density of the 132 bushing of the shaped powder metallurgy part is high, reaching 7.0g/cm3, and the hardness after sintering is also high, and the mandrel and the female mold are greatly affected during the shaping process. Under the repeated extrusion of the die, the residual austenite in the subsurface of the die is repeatedly deformed, resulting in dislocation accumulation and initiation of cracks. During the repeated extrusion process, the cracks expand until the surface is peeled off, forming Severe spall pit (1). In addition, the impurities in the powder—a variety of hard phase particles, plough on the surface of the mold during the mold shaping process, so that the surface of the mold is covered with furrows. Because the impurity particles are small, the furrows formed are shallow. The mandrel is scrapped due to oversize due to the combined action of spalling and ploughing.

    The microstructure of the mandrel made of GCr15 die steel undergoes the following changes during the cryogenic treatment (2) (3), and the amount of retained austenite decreases. The alloying elements in the retained austenite, especially the carbon element, play a role in strengthening the retained austenite, so more energy is required to promote the shearing mechanism to generate martensite. Cryogenic treatment is to use the degree of supercooling to increase martensite. The driving force for bulk transformation, as the cryogenic temperature decreases, the degree of subcooling increases, and the martensitic transformation becomes more complete. In the cooling process, the transformation speed of retained austenite to martensite does not depend on time, but is related to the degree of supercooling, that is, the amount of retained austenite is only related to the cryogenic temperature. In addition, cryogenic treatment can also precipitate fine carbides and refine the structure.

    Cryogenic treatment reduces the amount of retained austenite and increases the difficulty of crack initiation in the subsurface layer of the mandrel during extrusion. At the same time, due to the decrease in the amount of retained austenite, the precipitation of fine carbides and the refinement of the structure, the difficulty of ploughing is increased. . Therefore, after the mandrel is cryogenically treated, the ability to resist fatigue wear and abrasive wear is increased, thereby improving the life of the mandrel. If the cryogenic treatment temperature is high (higher than -160°C), the degree of undercooling is small, the energy for the transformation of retained austenite to martensite is insufficient, and the amount of retained austenite is large, which means that the hardness of the mold is almost unchanged. The mold life is not much improved. Cryogenic treatment at a lower temperature, as long as the holding time is enough to make the mandrel cool through (not less than 2h), the transformation of retained austenite to martensite is relatively complete, but the amount of fine carbides precipitated in martensite varies with the increased slowly with the extension of the holding time. Therefore, mold life also increases slowly with holding time. If it is considered that with the extension of the holding time, the cost of the cryogenic treatment of the mold also increases, then the most suitable holding time is 2 to 4 hours.

    3 Conclusion
    The failure mechanism of powder metallurgy parts shaping die is fatigue wear and abrasive wear. Cryogenic treatment of the mold can greatly improve its life. The best cryogenic temperature is -160℃~-196℃. The longer the holding time is, the longer the life of the mold will be. However, considering both the cost and the lifespan, it is appropriate to take 2 to 4 hours.

    Zhejiang Yuanzheng Technology

    Address: Room 1107, Building 1, Chenxin Building, Wuyang Sub-District, Deqing County, Zhejiang Province, China
    Tel: +86-572-8816606 8817606
    Mobile: +86-13967262286(Pan Xuewei)
    E-mail: sales@yzfm.com
    Website: http://www.isyv.cn

    Copyright(C)2022, Zhejiang Yuanzheng Technology Co., Ltd. All Rights Reserved. Supported by  ChemNet ChinaChemNet Toocle
    特级毛片A级毛片免费播放| 久草性视频| 老少配老妇老熟女中文普通话| 波多野结AV衣东京热无码专区| 2021少妇久久久久久久久久| 亚洲中文精品人人永久免费| 国产色婷婷五月精品综合在线| 国产精品久久久久无码AV| 2021少妇久久久久久久久久| 婷婷色一区二区三区| 人人妻人人澡人人爽欧美一区| 国产美女亚洲精品久久久综合| 国产精品无套在线观看| 娇妻被别人带去杂交| 国产精品老年自拍视频| yjizz国产在线视频网| 日日夜夜国产自偷自拍| 99久久久无码国产精品性| 一区二区三区四区在线| 美女啪啪无遮挡| 国产精品福利2020久久| 波多野结衣无码中文字幕在线观看一区二区| 在线国产毛片| 国产女人喷水视频| 人妻在线免费观看视频| 91蜜臀精品国产自偷在线| 精久久久久无码区中文字幕| H无码精品3D动漫在线观看| 成人免费A级毛片无码片2022| 国产精品毛片在线更新| 久久精品夜夜夜夜夜久久| 国产精品视频一区不卡| 亚洲精品无AMM毛片| 天堂中文在线资源| 国产成人综合日韩精品无码不卡| 国产美女被遭强高潮免费一视频| 亚洲 欧洲 无码 在线观看| 美女三级久久精品一区| 久久超碰色中文字幕超清| 日本中文字幕有码高清| 国产伦精品一区二区三区视频优播|